Abstract:Ball milled Ti/BN composite powder was prepared by high energy ball milling for 40 h, using Ti and BN (the molar ratio of Ti/BN is 3:2) as starting materials. The as-milled composite powder consists of TiN, Ti and amorphous phase. TiN formed while the milled powder was annealed at 400℃. The heat treatment at 700℃ led to the formation of TiB2 and TiB. The nanocrystalline Ti and amorphous phase converted to TiN and TiB2 when the powder was heated to 1300℃.