摘 要: | 攀钢钛业公司选钛厂电选尾矿含TiO2 10 .82 % ,采用湿式强磁粗选、摇床精选的工艺流程 ,可有效回收其中的钛铁矿 ,得到含TiO2 为 47.48%、回收率为 76.65 %的合格钛精矿。
|
关 键 词: | 钛铁矿 湿式强磁选 重选 尾矿 |
文章编号: | 1671-9492(2004)04-0027-03 |
修稿时间: | 2003年9月11日 |
STUDY ON COMPREHENSIVE UTILIZATION OF TITANIUM ELECTROSTATIC SEPARATION TAILING |
| |
Authors: | DAI Hui-xin WANG Yun-hua |
| |
Abstract: | The electrostatic separation tailing in Titanium Dressing Plant of Titanium Industry Branch of Panzhihua contains 10.82% TiO 2, for which the technological flow of wet high intensity magnetic roughing process and table concentration is adopted and of which the Titanium can effectively be recovered. Hence, the qualified Titanium concentrate can be attained, of which TiO 2 is 47.48% and the recovery is 76.65%. |
| |