摘    要:重点研究了注射成形Kovar 合金的脱脂及烧结工艺。结果表明:溶剂脱脂+热脱脂工艺能有效快速地实现粘结剂的完全脱除, 通过烧结后获得了25~400 ℃内平均热膨胀系数为5.75×10-6/ ℃的注射成形Kovar 合金封装盒体。金相显微组织及XRD 分析说明了合金主要以奥氏体(γ相)主相及少量的α相共同组成, 这种α相的存在是PIMKovar 合金热膨胀系数偏高的主要原因。

关 键 词:粉末注射成形  Kovar合金  热膨胀性  电子封装材料
文章编号:0253-6099(2004)05-0070-03
收稿时间:2004-04-27
修稿时间:2004-04-27

Study on Powder Injection Molding of Kovar Alloy
DUAN Bo-hua,ZHOU Xiao-hui,QU Xuan-hui ,,XU Zheng-zhou. Study on Powder Injection Molding of Kovar Alloy[J]. Mining and Metallurgical Engineering, 2004, 24(5): 70-72
Authors:DUAN Bo-hua  ZHOU Xiao-hui  QU Xuan-hui     XU Zheng-zhou
Affiliation:1. The State Key Laboratory for Powder Metallurgy, Central South University, Changsha 410083, Hunan, China;2.School of Materials Science and Engineering, Beijing University of Science &Technology, Beijing 100083, China
Abstract:The debinding and sintering process in the powder injection molding(PIM)of Kovar alloy has been investigated here.The results show that all the binder can be removed rapidly and effectively by the solvent debinding and thermal debinding, PIM Kovar alloy packing box with an average thermal expansion coefficient of 5.75 ×10-6/ ℃over the range of 25 ℃to 400 ℃ can be obtained after sintering.Both metallurgical microsructure and X-ray diffraction analysis show that the alloy is composed of austenititephase (γphase)and a little ferrite phase (αphase), while the existence of αphase mainly results in the higher thermal expanxion coefficient of PIM Kovar alloy.
Keywords:powder injection molding(PIM)  Kovar alloy  thermal expansion  electronic packaging material