摘    要:对红土镍矿堆浸搅拌浸出工艺进行了中试研究, 红土镍矿经洗矿分级后, +0.25 mm粗粒级矿石进行堆浸, -0.25 mm细粒级矿石常压搅拌浸出。结果表明 在堆高4 m, 酸耗700 kg/t, 浸出时间142 d的柱浸条件下, Ni累计浸出率约80%;在酸耗850 kg/t, 浸出时间3.5 h, 浸出温度90~95 ℃, 矿浆浓度26%的搅拌浸出条件下, Ni浸出率可以达到85%以上。

关 键 词:红土镍矿  堆浸  搅拌浸出  中试  
收稿时间:2014-04-17

Pilot Study on a Combined Process of Heap Leaching and Atmospheric Tank Leaching for Nickel Laterites
LIU Sanping,WANG Haibei,ZHANG Lei,ZOU Xiaoping. Pilot Study on a Combined Process of Heap Leaching and Atmospheric Tank Leaching for Nickel Laterites[J]. Mining and Metallurgical Engineering, 2014, 34(5): 97-99. DOI: 10.3969j.issn.0253-6099.2014.05.024
Authors:LIU Sanping  WANG Haibei  ZHANG Lei  ZOU Xiaoping
Affiliation:1.School of Materials & Metallurgy, Northeastern University, Shenyang 110819, Liaoning, China; 2.Beijing General Research Institute of Mining and Metallurgy, Beijing 100160, China
Abstract:A pilot experiment was conducted on processing of nickel laterites with a combined process consisting of heap leaching and atmospheric tank leaching(ATL). After stages of scrubbing and screening, the ore was classified into two size fraction, one with size of +0.25 mm as feed to heap leach and another size of -0.25 mm as feed to atmospheric tank leach. It was found that the accumulated extraction rate of Ni was about 80% after column leaching with heap height of 4 m, acid consumption at 700 kg/t and leaching time of 142 d. However, the extraction rate of Ni after ATL could exceed 85% with acid consumption of 850 kg/t, leaching temperature of 90~95 ℃ and leaching time of 3.5 h, at pulp density of 26%.
Keywords:nickel laterites  heap leaching  atmospheric tank leaching ( ATL)  pilot study
本文献已被 CNKI 万方数据 等数据库收录!
点击此处可从《矿冶工程》浏览原始摘要信息
点击此处可从《矿冶工程》下载全文
设为首页 | 免责声明 | 关于勤云 | 加入收藏

Copyright©北京勤云科技发展有限公司  京ICP备09084417号