摘    要:某锌浸出渣中含银228.24g/t,该浸出渣具有粒度细、酸性强、银的物象分布复杂等特点。针对该浸出渣,实验采用添加乳化煤油选择性絮凝矿浆中的微细颗粒增大表观粒度,并通过洗矿调节矿浆PH值以及降低矿浆中锌离子的浓度。实验结果表明:在PH=5.47的条件下,以六偏磷酸钠为分散剂,丁铵黑药为捕收剂,MIBC为起泡剂,采用一粗二扫浮选工艺流程,可获得含银3439g/t,回收率为76.54%的浮选精矿。

关 键 词:锌浸出渣  银浮选  综合回收  二次资源
收稿时间:2018/5/14 0:00:00
修稿时间:2018/5/21 0:00:00

A preliminary study of the silver flotation experiment from the zinc leaching residue
Authors:Chen Li  Jun-wei Han  Wei Liu  Tian-fu Zhang and Lin Zhu
Affiliation:School of Minerals Processing and Bioengineering ,Central South University,School of Minerals Processing and Bioengineering ,Central South University,School of Minerals Processing and Bioengineering ,Central South University,School of Minerals Processing and Bioengineering ,Central South University,School of Minerals Processing and Bioengineering ,Central South University
Abstract:There is 228.24g/t silver in the zinc leaching residue, which has the characteristics of fine particle size, high acidity and complicated distribution of sliver phase. Aimed the leacfhing residue, this experiment used the emulsified kerosene to flocculate the tiny particles for increase the apparent granularity of the particles in the pulp, in addition, by means of different washing times of the ore to adjust the pH of the pulp and eliminate the adverse effect of zinc ions on flotation. The result indicated that, adjusting the pulp pH in 5.47 conditions, adding sodium hexametaphosphate as dispersant, ammonium dibutyl dithio phosphate as the collector and MIBC as foaming agent and using a flowsheet of one stage of roughing and two stages of scavenging for the silver flotation can obtained a silver concentrate with silver content and recovery of 3439g/t and 76.54%.
Keywords:zinc leaching residue  flotation  comprehensive recovery  secondary mineral resources